HDG vs Dacromet: the cost maths behind salt spray data
Why do Australian projects specify HDG while European solar prefers Dacromet? Lay out the 500h, 720h and 1000h data and the answer is a cost question, not a chemistry one.
The most common buying mistake is treating salt spray hours as the only metric. In reality it answers one question only: how long until red rust appears in a neutral salt spray chamber. It does not tell you what happens three years into a coastal installation, nor whether the coating cracks when you torque the bolt.

1. Three data sets side by side
| Finish | Typical coating | NSS to red rust | Cost index | Hydrogen risk |
|---|---|---|---|---|
| Zinc plated | 8–12 μm | 48–96 h | 1.0 | High — de-embrittlement bake needed |
| Dacromet / zinc-flake | 6–10 μm | 720–1000 h | 1.6–2.2 | Low |
| Hot-dip galvanised | 45–86 μm | 500–1000 h | 1.3–1.8 | None — thread clearance required |
| Stainless 304/316 | — | >2000 h | 4–8 | None |
Note that HDG and Dacromet overlap on salt spray. On paper they draw. What separates them is coating thickness, behaviour after mechanical damage, and how forgiving each is during assembly.
2. HDG wins on thickness — and loses on it
An 86 μm layer means there is still margin after a scratch. Site handling, transport damage and on-site cutting are all tolerated better — which is why consultants on Australian and Middle Eastern steel projects insist on it.
Thickness brings two side effects: threads must be cut with a clearance (an M12 becomes 6AZ) or the nut will not run on; and the finish is coarse with visible colour variation, which rules it out for retail packaging.
3. Dacromet wins on thinness and hydrogen
For grade 10.9 and above, zinc plating requires a de-embrittlement bake (200℃ for four hours or more) or delayed fracture risk climbs. Dacromet is a water-based zinc-flake coating cured by sintering and produces no hydrogen — the main reason automotive and solar racking use it in volume.
The other overlooked point is galvanic coupling. Aluminium rail plus zinc-plated steel in a wet environment forms a couple and the aluminium is sacrificed. The aluminium flakes in Dacromet sit closer to the rail potential — an implicit reason European solar specifies it.
4. How to choose: by condition, not by price
- Within 1 km of the coast, concrete substrate, on-site cutting → HDG 86 μm
- Grade 10.9+, fatigue-loaded → Dacromet; never zinc plating
- Aluminium racking, visible surfaces → Dacromet or zinc-flake
- Indoor dry, cost-sensitive → zinc plated with de-embrittlement
- Chemical plant or immersion service → SS316, or HDG plus a top coat
Want this mapped to your project? Send the substrate, corrosivity category and annual volume — we will recommend a finish against EN ISO 12944 and attach the matching salt spray report.
Want these figures checked against your job?
Send substrate, corrosivity category, annual volume and destination port — we reply with a quote including the standard and finish recommendation.
Related reading
- Case studyCase: from one trial container to six a year in AustraliaNot by cutting price. Three steps: a salt spray comparison video, a sample kit, then private-lab…
- SelectionAnchor selection: three traps in concrete strength, edge distance and embedmentA wedge anchor is not universal. The same M12 can differ 40% in pull-out between C20 and C40, an…